무기성 순환자원의 수소 활성화 및 이산화탄소 분해
Hydrogen Activation and Carbon Dioxide Decomposition Using An Inorganic Recycling Resource
- 한국응용과학기술학회 (구.한국유화학회)
- 한국응용과학기술학회지
- 한국유화학회지 제26권 제4호
-
2008.12483 - 490 (8 pages)
- 5
This research was conducted to estimate the characteristics of carbon dioxide decomposition using an inorganic sludge. The inorganic sludge was composed of high amount (66.8%) of Fe2O3. Hydrogen could be reduced with 0.247, 0.433, 0.644, and 0.749 at 350, 400, 450, and 500℃, respectively. The carbon dioxide decomposition rates at 250, 300, 350, 400, 450, and 500℃ were 32, 52, 35, 62, 75, and 84%, respectively. High temperature led to high reduction of hydrogen and better decomposition of carbon dioxide. The specific surface area of the sludge after hydrogen reduction was higher than that after carbon dioxide decomposition. The specific surface area of the sludge was more decreased with increasing of temperature.
1. 서 론
2. 실험재료 및 방법
3. 결과 및 고찰
4. 결 론
감사의 글
참고문헌