학술저널
Specimens of seven hardwood species were heat-treated at three temperature levels of 170, 190 and 210°C. Their FSP’s were measured by the volumetric swelling method and com-pared with the control’s. Within a species the FSP decreases as the temperature of heat treat-ment increases. The FSP’s of the controls range from 26.1 to 29.6%, while those of the speci-mens heat-treated at 210°C from 16.9 to 21.8%. There were no difference of basic density be-tween the heat-treated and control specimens. The color indexes of ash and beech specimens were measured using a colorimeter. It was revealed that the temperature of heat treatment af-fected on the color more than the treatment time.
Ⅰ. 서론
Ⅱ. 재료 및 방법
Ⅲ. 결과 및 고찰
Ⅳ. 결론
사사
참고문헌
(0)
(0)